性能项目 |
试验条件[状态] |
测试方法 |
测试数据 |
数据单位 |
物理性能 |
比重 |
|
ASTMD792A |
1.28 |
g/cm³ |
物理性能 |
密度 |
|
ISO1183/A |
1.28 |
g/cm³ |
机械性能 |
TensileStrength2(2.00mm,CompressionMolded) |
|
ASTMD638 |
10.0 |
MPa |
机械性能 |
拉伸应力(屈服,2.00mm,模压成型) |
|
ISO527-2/2/500 |
10.0 |
MPa |
机械性能 |
TensileElongation(Break,2.00mm,CompressionMolded) |
|
ASTMD638 |
780 |
% |
ELASTOMERS |
弹性体 |
|
TestMethod |
NominalValue |
Unit |
ELASTOMERS |
撕裂强度3 |
|
ASTMD624 |
31.0 |
kN/m |
ELASTOMERS |
TearStrength4,5(2.00mm) |
|
ISO34-1 |
31 |
kN/m |
硬度 |
DurometerHardness(ShoreA,15sec,2.00mm,CompressionMolded) |
|
ASTMD2240 |
67 |
|
硬度 |
ShoreHardness(ShoreA,15sec,2.00mm,CompressionMolded) |
|
ISO868 |
67 |
|
热性能 |
ColdFlexibility(-30°C) |
|
|
Pass |
|
老化 |
ChangeinTensileStrengthinAir(80°C,1000hr) |
|
ASTMD573 |
2.2 |
% |
老化 |
ChangeinTensileStrengthinAir(80°C,1000hr) |
|
ISO188 |
2.2 |
% |
老化 |
ChangeinUltimateElongationinAir(80°C,1000hr) |
|
ASTMD573 |
14 |
% |
老化 |
ChangeinTensileStrainatBreakinAir(80°C,1000hr) |
|
ISO188 |
14 |
% |
老化 |
ChangeinMassinAir(80.0°C,1000hr) |
|
ASTMD573 |
0.53 |
% |
老化 |
ChangeinMassinAir(80.0°C,1000hr) |
|
ISO188 |
0.53 |
% |
ADDITIONAL INFORMATION |
补充信息 |
|
TestMethod |
NominalValue |
Unit |
ADDITIONAL INFORMATION |
ColorStability6(98to102°C) |
|
MultipleStandards |
5.00 |
|
ADDITIONAL INFORMATION |
FloridaWeathering |
--7 |
|
>0.470 |
|
ADDITIONAL INFORMATION |
FloridaWeathering |
--8 |
|
>1.96 |
|
ADDITIONAL INFORMATION |
StainResistance |
--9 |
|
Pass |
|
ADDITIONAL INFORMATION |
StainResistance |
--10 |
|
Pass |
|
ADDITIONAL INFORMATION |
StainResistance |
XenonWeatherometer11 |
|
>4.50 |
|